PICTURES

BUILDING DATA

ENVIRONMENTAL DATA

CAUSATION

REMEDIATION

 

 

HDB indoor
Location Yio Chu Kang
Orientation North-South
Materials Black veneer wood and teakwood
RH indoor 62.9%
Surface Moisture 20%
Surface Temperature 24°C
Wind velocity indoor 0-0.2 m/s
Stain types White patches form rounding form
Stain size Irregular form
Stain location all the wardrobe door and bedroom door
   
Wind Speed 0.1-0.3 m/s
Wind Direction East-West
Ambient Temperature 29.2°C
RH 62%
  • The outdoor conditions High humidity, windy, dense plantation, causes the moulds spore concentration are higher than other area. High humidity leads to a prone condition for HDB units to be attacked by moulds growth.
  • Furniture moisture contents The black veneer wood furniture and teakwood door have quite high moisture content 20% (above the average standard). It is concluded that the furniture is categorized “wet” and need to be dry up.
    • Remove moulds growth by wiping or vacuuming the surface. Vacuuming should be conducted with a wet –dry vacuum and the filter should be replaced. Those cleaning should be done outdoor.